Illustrated title card for the guide: QIDI Q2 PAHT-CF Settings, Nozzle Size and Drying
setup

QIDI Q2 PAHT-CF Settings, Nozzle Size and Drying

Set up QIDI PAHT-CF on the Q2 with a wear-resistant nozzle, the correct drying cycle, direct feed from a dry box, and a glued textured PEI plate.

For QIDI PAHT-CF on the Q2, dry the spool at 80–100 °C for 4–6 hours, then print with a 0.4 mm hardened-steel nozzle at 300–320 °C and a glued bed at 70–90 °C. QIDI PAHT-CF printing guide

Choose the nozzle

NozzleWhen to use it
Stock 0.4 mmThe Q2 comes with a 0.4 mm bimetal nozzle. Q2 specs QIDI describes the Q2 nozzle as hardened steel and lists 0.4 mm among the recommended sizes for PAHT-CF. QIDI filament guide
Optional 0.6 mm Q2 specsIf the 0.4 mm nozzle clogs, QIDI recommends moving to 0.6 mm. Choose a hardened-steel, bimetal or tungsten carbide bimetal nozzle. QIDI filament guide

QIDI advises against brass, copper-plated and 0.2 mm bimetal nozzles for this spool. QIDI filament guide

For other Q2 hardware details, see the Q2, Q2C and Q1 Pro specs comparison.

Dry the spool and feed it directly

  1. Dry the spool in a blast drying oven at 80–100 °C for 4–6 hours. QIDI drying instructions
  2. Put the spool in a sealed dry box with desiccant. Keep it below 15% relative humidity during the print. QIDI drying instructions
  3. Feed the filament straight from the dry box to the Q2, bypassing the QIDI BOX feed path. Keep the printer enclosure closed during printing. QIDI feed and chamber guidance

QIDI lists its PAHT-CF as unsupported for printing through the QIDI BOX. QIDI BOX specifications

For other spools, see the QIDI BOX compatibility matrix.

Set up the textured PEI plate and print temperatures

The Q2 comes with a dual-sided textured PEI plate. Q2 specs

  1. Apply glue to the PEI surface with a glue stick. QIDI build plate guidance
  2. For the stock nozzle, OrcaSlicer lists the Qidi Q2 0.4 nozzle printer profile. OrcaSlicer 0.4 mm machine profile
  3. With Support multi bed types enabled in printer settings, choose Textured PEI Plate in the bed-type dropdown. Set the temperature for that plate in the filament settings. OrcaSlicer bed-type documentation
SettingQIDI PAHT-CF recommendation
Nozzle temperature300–320 °C
Bed temperature70–90 °C with glue
Part cooling fanOff, per QIDI’s technical data sheet
Print speed30–120 mm/s

QIDI print settings

Evidence and limits. QIDI’s material and hardware documentation, OrcaSlicer’s main-branch Q2 machine profile, and its bed-type documentation were checked on November 28, 2026. The settings cover QIDI’s PAHT-CF spool on the Q2. No hands-on testing was performed for this guide.

Sources

  1. QIDI PAHT-CF printing guide
  2. QIDI Q2 technical specifications
  3. QIDI BOX technical specifications
  4. OrcaSlicer Q2 0.4 mm machine profile
  5. OrcaSlicer Wiki on printable space and bed types